Mechanical Properties of Hemp Fiber Filled Polypropylen

Properties
PP + 30% HF
Young Modulus (GPa)
1.8
Re (Mpa) 25 mm/min
19
Rm (Mpa) 25 mm/min
25
A (%) 25 mm/min
>260
MFI (g/10 min) 2.16 kg/230°C
6.5
Hardness (Shore D)
68
Density (kg/m3)
980
Barrel Temperature (°C)
180-230
Mould Temperature (°C)
40-70
Drying Temperature (°C)
60-80 (3h)
Shrinkage (%)
1.8
Resistivity (ohm cm)
>10.12
Vicat Softening Point (°C)
100